Why Pots Crack (and How to Stop It)

S-cracks, rim cracks, dunting and handles popping off: the causes and the fixes.

S-cracks in the base

Caused by an uncompressed floor and uneven drying. Compress the floor while throwing, and dry pots upside down once they can take it.

Cracks where handles join

The handle and body dried at different rates. Attach at the same leather-hard stage, score and slip well, and slow drying under plastic.

Rim cracks

Rims dry first. Compress the rim while throwing and cover rims with plastic during early drying.

Dunting (cracks during firing)

Cooling cracks happen at quartz inversion (around 1,063 °F / 573 °C) or cristobalite inversion (around 435 °F / 225 °C) when cooling is too fast or walls are uneven. Even wall thickness and slower cooling help.